(1)将已浸水一昼夜的试件从水中取出,用软的旧布吸试件表面的可见自由水,并称试件的质量m4。dv4©bbs.3c3t.comÓ5VG&0]S¢
dv4©bbs.3c3t.comÓ5VG&0]S¢
dv4©bbs.3c3t.comÓ5VG&0]S¢
dv4©bbs.3c3t.comÓ5VG&0]S¢
(2)用游标卡尺量试件的高度h1,准确到0.1mm。dv4©bbs.3c3t.comÓ5VG&0]S¢
dv4©bbs.3c3t.comÓ5VG&0]S¢
dv4©bbs.3c3t.comÓ5VG&0]S¢
dv4©bbs.3c3t.comÓ5VG&0]S¢
(3)将试件放到路面材料强度试验仪的升降台上(台上先放一扁球座),进行抗压试验。试验过程中,应使试dv4©bbs.3c3t.comÓ5VG&0]S¢
dv4©bbs.3c3t.comÓ5VG&0]S¢
dv4©bbs.3c3t.comÓ5VG&0]S¢
dv4©bbs.3c3t.comÓ5VG&0]S¢
件的形变等速增加,并保持速率约为lmm/min记录试件破坏时的最大压力P(N)。dv4©bbs.3c3t.comÓ5VG&0]S¢
dv4©bbs.3c3t.comÓ5VG&0]S¢
dv4©bbs.3c3t.comÓ5VG&0]S¢
dv4©bbs.3c3t.comÓ5VG&0]S¢
(4)从试件内部取有代表性的样品(经过打破)测定其含水量w1。dv4©bbs.3c3t.comÓ5VG&0]S¢
dv4©bbs.3c3t.comÓ5VG&0]S¢
dv4©bbs.3c3t.comÓ5VG&0]S¢
dv4©bbs.3c3t.comÓ5VG&0]S¢
(5).计算试件的无侧限抗压强度Rc。Rc0.95(=Rc-1.645S)。允许误差:若干次平行试验的偏差系数Cv(%)应符dv4©bbs.3c3t.comÓ5VG&0]S¢
dv4©bbs.3c3t.comÓ5VG&0]S¢
dv4©bbs.3c3t.comÓ5VG&0]S¢
dv4©bbs.3c3t.comÓ5VG&0]S¢
合下列规定:小试件 不大于10%,中试件 不大于15%,大试件 不大于20%dv4©bbs.3c3t.comÓ5VG&0]S¢