不锈钢304牌号鉴定1、案例背景Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘
该不锈钢产品的使用领域的食品接触材料领域,产品主要用于制作汤锅、水壶等。委托方要求分析该材料是否符合美国标准ASTM  A276-2013 304牌号的要求,以确定其所使用的材料是符合《GB 9684-88 不锈钢食具容器卫生标准》条款。Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘
Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘
Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘
2、分析方法简述Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘
Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘
Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘
a、对样品进行XRF半定量分析,分析结果如下:Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘
Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘
Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

元素Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

MnÜ7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

CrÜ7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

NiÜ7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

CuÜ7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

MoÜ7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

含量Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

1.05%Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

18.01%Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

8.02%Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

0.10%Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

0.23%Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘
Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘
Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘
Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘
从XRF定性半定量结果上分析,初步可以判定该材料应属于GB 9684-88所规定的奥氏体不锈钢。于是参考不锈钢分析标准对材料进行准确定量分析。Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘
Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘
Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘
b、依据《GB/T 20123-2006 钢铁 总碳硫含量的测定 高频感应炉燃烧后红外吸收法(常规方法)》,采用纳克CS3000碳硫分析仪对该材料进行C和S含量分析,结果如下:Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘
Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘
Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

元素Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

CÜ7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

SÜ7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

含量Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

0.065%Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

0.018%Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘
Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘
c、依据《JIS G1258-2-2007 中文版 铁及钢—ICP发光光谱分析方法—第2部:锰、镍、铬、钼、铜、钨、钒、钴、钛及铌定量方法—硫酸磷酸分解法》,采用OPTIMA8000对该材料进行Si、Mn、P、Cr、Ni、Cu、Mo等元素进行定量分析,结果如下:Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

元素Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

SiÜ7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

MnÜ7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

PÜ7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

CrÜ7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

NiÜ7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

MoÜ7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

CuÜ7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

含量Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

0.587%Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

1.15%Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

0.035%Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

18.28%Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

8.34%Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

0.43%Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

0.21%Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘
Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘
Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘
Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘
Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘
3、结果分析与讨论Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘
通过对该不锈钢材料进行成分分析,并对照ASTM A276-2013 304不锈钢材料成分含量要求发现,该不锈钢材料符合304不锈钢要求,属于《GB 9684-88 不锈钢食具容器卫生标准》所要求的奥氏体不锈钢。Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

元素Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

材料成分含量Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

304牌号成分要求Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

CÜ7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

0.065%Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

0.08%Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

SÜ7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

0.018%Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

0.030%Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

SiÜ7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

0.587%Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

1.00%Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

MnÜ7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

1.15%Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

2.00%Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

PÜ7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

0.035%Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

0.045%Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

CrÜ7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

18.28%Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

18.0%-20.0%Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

NiÜ7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

8.34%Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

8.0%-11.0%Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

CuÜ7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

0.21%Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

MoÜ7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

0.43%Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

FeÜ7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

余量Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘
Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘
Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘
Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘
Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

4、参考标准Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

  GB/T 20123-2006 钢铁 总碳硫含量的测定 高频感应炉燃烧后红外吸收法(常规方法)Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

  JIS G1258-2-2007 中文版 铁及钢—ICP发光光谱分析方法—第2部:锰、镍、铬、钼、铜、钨、钒、钴、钛及铌定量方法—硫酸磷酸分解法Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘

Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘
Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘
Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘
Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘
Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘
分享 转发
TOP
2#

这是做什么的Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘
TOP
3#

这不叫鉴定,叫检测吧Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘
TOP
4#

对呀Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘
www.3c3t.net   www.3c3t.comÜ7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘
TOP
5#

来这里看看了Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘
TOP
6#

快来看看了Ü7¾Kî}Í1Šbbs.3c3t.comÚu±t€‘p‚‘
TOP
发主话题 回复该主题